At a glance: In a submerged MBR, hollow fibres hang in activated sludge and are shaken by air bubbles all day. An unsupported fibre can break, and a broken fibre lets sludge into the permeate. A braided reinforced fibre avoids this: a thin membrane layer is coated on a hollow braided tube, so the braid carries the load and the membrane does the filtering. Theway's hollow fibre MBR modules use reinforced fibre.

Theway hollow fibre MBR module

How a reinforced fibre is made

  1. Braid. Polymer yarn, usually polyester, is braided into a hollow tube. The braid gives the fibre its size and its strength.

  2. Coating. The braid is drawn through a coating spinneret, where a polymer solution, typically PVDF, is laid evenly over the outside.

  3. Phase inversion. The coated braid enters a water bath and the coating sets as a porous membrane layer, anchored in the outer yarns, by the same mechanism as NIPS.

  4. Washing and finishing. Solvent and additives are washed out, and the fibre is treated and wound for potting.

The depth to which the coating enters the braid matters. Too shallow and the layer can peel; too deep and it blocks the braid and lowers flow. Getting this right is most of the skill in making reinforced fibre.

Unsupported and reinforced fibres compared

Aspect

Unsupported hollow fibre

Braided reinforced fibre

What carries the load

The membrane polymer

The braid

Breaking load

Low

Many times higher

Under air scour and sludge

Can break, mostly near the potting

Rarely breaks

If it fails

Fibre breaks and sludge reaches the permeate

Coating damage, if any

Backwash

Within the datasheet pressure

Low pressure, so the coating stays bonded

Typical use

Pressurised UF modules

Submerged MBR

What to check in an MBR fibre

  • Strength: the breaking load of the fibre, and how the coating is held to the braid.

  • Pore size: MBR fibres are microfiltration or loose ultrafiltration. Theway's TW-MBR56-40 element, for example, uses PVDF hollow fibre rated at 0.05 µm.

  • Operating limits: flux, transmembrane pressure, MLSS and air flow on the datasheet.

  • Cleaning: the sodium hypochlorite and acid strengths the membrane accepts.

For the choice between fibre and plate, see flat sheet or hollow fibre MBR. Theway also makes flat sheet MBR and Surge 500T modules for ZeeWeed 500D tanks.

Questions

Why do MBR fibres break?

Aeration keeps the fibres moving for years, and the stress gathers where they enter the potting. Sludge, rags and hair add to it. An unsupported fibre fails there first.

Can a reinforced fibre be backwashed?

Yes, at the low pressure given on the datasheet. Too high a backwash pressure can lift the coating from the braid.

Do pressurised UF modules need reinforced fibre?

Not usually. They work in clean housings without sludge or constant movement, so a well-made unsupported fibre, or a multi-bore fibre such as Septabore, is strong enough.